National Electroless Nickel - ISO American Global Standards

Specifications & Properties

Medium Phosphorus Electroless Nickel


Medium Phosphorus Electroless Nickel Our Medium Phosphorus Electroless Nickel process meets the requirements of ASTM B733 class V, AMS 2404, mil C26074 (all revisions), and ISO 4527. The coating conforms to the requirements of ELV Directive 2000/53/EC, WEEE 2002/96/EC, RoHS 2002/95/EC and NSF/ANSI 51-2005. IMDS number 32696178 (mid-P EN)


MEDIUM PHOSPHOROUS PHYSICAL PROPERTIES Typical Result
Phosphorus Content, wt, % 7 to 10
Melting Point (eutectic) 1560 to1620 °F
850-880 °C
Coefficient of Thermal Expansion, °m/(mK) 13 to 15
Thermal Conductivity, W/(mK) 40 to 45
Electrical Resistivity μΩ/ cm 50 to 100
Magnetic Properties Non-Magnetic (>8.5%P)
Hardness, Vickers hardness HV0.1, 100 g load, 40 μm deposit, steel
As plated 520 to 580
Heat Treated @
16 hr., 535 °F (280 °C) 920 to 980
4 hr., 660 °F (350 °C) 920 to 980
1 hr., 750 °F (400 °C) 920 to 980
Wear Properties, Taber Abraser Wear Test, Index Value weight loss mg/1000 cycles CS 10
As Plated 15 to 18
Heat Treated @ 1 hr., 750 °F (400 °C) 4 to 8
Corrosion Related Properties (25 μm thickness; Rz 1.5 μm; base material St 52.3)
EN 50021 SS (hr.) >500
EN 50021 ESS (hr) >150
EN 50018 2.0I SO2 cycles 3 to 8
Nitric Acid Test
Conc. Nitric acid 63% wt. 30 sec. room temp. 1 ml Fail*
50% HCl, 3 min. room temp. 1 mil steel Pass*







Your satisfaction is our business!